type: "Article"
title: "Comparative study of two seals made of FKM and EPDM"
description: "Case study Comparative study of two seals made of FKM and EPDM One of our customers encountered problems with the nature of their joints. Accueil • Blog • Comparative study of two seals made of FKM and EPDM The problem?..."
resource: "https://filab.fr/en/blog/2025/12/comparative-study-of-two-seals-made-of-fkm-and-epdm/"
tags: ["Case study", "Characterization of Materials", "Polymer", "EN", "pll_691f0c5b58403"]
timestamp: "2026-03-10T13:08:32Z"
published: "2025-12-02T07:05:35Z"
language: "en"
author: "bwa"
---

# Comparative study of two seals made of FKM and EPDM

Case study
# Comparative study of two seals made of FKM and EPDM

 One of our customers encountered problems with the nature of their joints. [Home](https://filab.fr) • [News](https://filab.fr/?post_type=post) • Comparative study of two seals made of FKM and EPDM
## The problem?

**As part of its industrial boiler production activities, one of our customers is currently involved in a dispute with its supplier following a labeling error on valves equipped with sleeves.
In order to remove any doubt about the conformity of the materials received, it wishes to confirm that the seals inside the valves are indeed made of FKM (fluoroelastomer)—a material known for its high chemical and thermal resistance—and not EPDM (ethylene propylene diene monomer), which is more suitable for aqueous or less aggressive environments, as indicated on the label.**

In order to carry out this study, FILAB developed an analytical approach using Fourier Transform Infrared Spectroscopy (FTIR), a chemical analysis technique that can identify the molecular structure of many materials, particularly for the study of polymers.

## Summary

 01 Determine the physical and chemical composition of the valve sleeve seal. [](#cont-01) 02 Comparative study of the two joints [](#cont-02) 03 Conclusion of the comparative study [](#cont-03)   01
## Determine the physical and chemical composition of the valve sleeve seal.

**Objective:**

This step aims **to confirm that the valve and its [seal](https://filab.fr/en/our-services/our-analysis-services/polymer-materials-analysis-laboratory/laboratory-analysis-of-joint.md) have the necessary characteristics to transport the fluid passing through the valve**, namely a synthetic gas produced by the carbonization of wood, a complex mixture containing corrosive and volatile compounds.
Another purpose of this study **is to verify that the seal has not deteriorated during use**.

![](https://filab.fr/wp-content/uploads/2025/09/ecovadis-81.png)

**Approach:**

For this study, the technique used is [Fourier Transform Infrared Spectroscopy (FTIR)](https://filab.fr/en/our-technical-resources/laboratory-analysis-ftir-spectroscopy.md) between 4000 and 400 cm-1. This technique involves **subjecting the sample to infrared radiation**: each type of chemical bond absorbs a specific wavelength, which provides a true **"chemical fingerprint"** of the material.

**With this analytical technique, the material is identified in two stages.**

The characteristic peaks are extracted to search for the corresponding bonds in reference tables. The continuous spectrum is then compared to a spectral database, which allows the nature of the material to be determined accurately through maximum correspondence calculations.

At the same time, FTIR analysis allowed us to check for any abnormal degradation of the seal by comparing used samples.

   02
## Comparative study of the two joints - compliance study

Spectroscopic analysis of the sample reveals several characteristic absorption bands, including C-F and C-C bond stretching (between 1393 and 1080 cm⁻¹), CF and CH vibrations (between 829 and 720 cm⁻¹), and CF₂ group deformations groups (around 634 and 607 cm⁻¹).
These signals are characteristic of a fluorinated [elastomer](https://filab.fr/nos-prestations/analyse/analyse-plasturgie-analyse-polymeres/laboratoire-analyse-caoutchouc-elastomere.md). The results as a whole therefore lead to the conclusion that the seal analyzed is made of a material of the **FKM (fluoroelastomer)** type, commonly used for its chemical and thermal resistance properties.

Comparison of the FTIR spectrum of the customer sample (blue) and a "FKM" reference (black).

![](https://filab.fr/wp-content/uploads/2025/09/Capture-decran-2025-09-25-094218-300x168.png)

In addition, to assess any abnormal degradation, a comparison was made between samples of seals in service and new samples. The results show that the used seal retains the same chemical characteristics as the new seal: **no alteration or degradation of the material was detected**.

   03
## Conclusion of the comparative study

Thanks to the analysis carried out using **Fourier Transform Infrared Spectroscopy (FTIR)**, our teams were able to confirm the [**exact nature of the polymer**](https://filab.fr/en/our-services/our-analysis-services/polymer-materials-analysis-laboratory/identification-of-the-nature-of-a-polymer.md) used in the seals: it was indeed **FKM (fluoroelastomer)** and not **EPDM**, as suggested by the supplier's labeling.

This precise identification made it possible to **remove any doubt about the conformity of the parts** and rule out the possibility of a [material](https://filab.fr/en/our-services/our-analysis-services/polymer-materials-analysis-laboratory.md) error.
Furthermore, a comparison between **new and used seals** showed **no significant chemical degradation**: the material retained all its properties over time.

Our customer was able to **continue production without concern**, with no impact on the safety or performance of its facilities.
This study perfectly illustrates how [**material characterization**](https://filab.fr/en/our-services/our-analysis-services/polymer-materials-analysis-laboratory/laboratory-material-testing) goes beyond simple testing to **ensure industrial safety** and **maintain trust between partners.**

  Need help? Contact our team [](#filab-contact-form)
## Other case studies you may be interested in

### Comparison of the quality of a metal oxide coating for a ski mask using AFM

 The customer wants to compare the quality of metal oxide for his ski mask. [Learn more +](https://filab.fr/en/blog/2025/12/metal-oxide-coating-on-ski-goggles.md)
### XPS coating

 Comparative study of multilayer coatings on zirconium tubes using XPS [Learn more +](https://filab.fr/en/blog/2025/12/study-of-the-purity-of-a-coating-layer-using-xps.md)
### Rouging phenomenon

 With its excellent properties, stainless steel has become indispensable in many fields: everyday objects, medicine, surgery, automotive, aeronautics, mechanical industries, etc. However, many industrial stainless steel installations are affected by the phenomenon of rouging. [Learn more +](https://filab.fr/en/blog/2025/12/how-did-filab-help-one-of-its-customers-understand-a-rouging-phenomenon-in-stainless-steel.md) [View all our case studies](https://filab.fr/en/blog-filab.md)
## Services related to the case study

 [## Metal analysis in black mass](https://filab.fr/en/metal-analysis-in-black-mass.md)   [![avis filab](https://filab.fr/wp-content/themes/astra-child/templates/assets/img/avis-verifies.svg) 5/5 ![note filab](https://filab.fr/wp-content/themes/astra-child/templates/assets/img/stars.svg)](https://www.avis-verifies.com/avis-clients/filab.fr)
## Laboratory specializing in analysis and expertise for industrial companies

 ![More than 140 people](https://filab.fr/wp-content/uploads/2024/10/collaborateurs-1.svg) More than 140 people at your service ![5200 m² laboratory](https://filab.fr/wp-content/uploads/2024/10/labo.svg) 5200 m² laboratory + 99% of services are provided in-house ![Accredited laboratory](https://filab.fr/wp-content/uploads/2024/10/ISO-17025-1.svg) Accredited laboratory COFRAC ISO 17025 ![+2200 clients](https://filab.fr/wp-content/uploads/2024/10/clients.svg) +2200 clients in France and abroad
### Contact us

 Our services are reserved for professionals.  [![phone](https://filab.fr/wp-content/themes/astra-child/templates/assets/img/form/phone.svg) Call
 us +33 (0)3 80 52 32 05](tel:+33380523205) [![location](https://filab.fr/wp-content/themes/astra-child/templates/assets/img/form/location.svg) Visit us 80 rue Jean-Louis Auguste Petitjean
 21850 - Saint Apollinaire - FRANCE](https://www.google.com/maps/place/Filab/@47.317329,5.076545,15z/data=!4m6!3m5!1s0x47f29e6ab37d6a1d:0xa2cc1016c4f74422!8m2!3d47.317793!4d5.0767354!16s%2Fg%2F1v3gr7f0?entry=ttu) [![mail](https://filab.fr/wp-content/themes/astra-child/templates/assets/img/form/envelope.svg) Contact
 us contact@filab.fr](mailto:contact@filab.fr?subject=%5BVotre%20demande%20:%20How%20did%20FILAB%20help%20one%20of%20its%20customers%20understand%20a%20rouging%20phenomenon%20in%20stainless%20steel?%20en%20%5D) For complaints: all complaints must be sent by mail to contact@filab.fr or by contacting the person who signed the report. The complaint handling procedure is available upon request. In the event of a complaint concerning the laboratory's activities, the customer may be notified of the complaint's handling.