title: "How FILAB helped one of its customers understand the yellowing phenomenon of a #silicone?"
description: "Case study Yellowing of silicone: expertise in action Our customer encountered yellowing issues with a batch of material. Accueil • Blog • Yellowing of silicone: expertise in action How FILAB helped one of its customers understand the yellowing of a..."
resource: "https://filab.fr/en/blog/2025/12/how-filab-helped-one-of-its-customers-understand-the-yellowing-phenomenon-of-a-silicone/"
tags: ["Case study", "EN", "pll_692040b83ad06"]
timestamp: "2026-01-22T13:12:22Z"
published: "2025-12-02T07:05:18Z"
language: "en"
author: "bwa"
---

# How FILAB helped one of its customers understand the yellowing phenomenon of a #silicone?

Case study
# Yellowing of silicone: expertise in action

 Our customer encountered yellowing issues with a batch of material. [Home](https://filab.fr) • [News](https://filab.fr/?post_type=post) • Yellowing of silicone: expertise in action
## How FILAB helped one of its customers understand the yellowing of a silicone compound.

**[Silicones](https://filab.fr/en/our-services/our-analysis-services/polymer-materials-analysis-laboratory/laboratory-analysis-silicone.md) are now widely used in various fields thanks to their remarkable physical and chemical properties, such as excellent thermal stability, high resistance to oxidation and hydrolysis, and excellent gas permeability. Finally, their non-toxicity and chemical inertness allow many types of silicones to be used in cosmetics, dentistry, medicine, surgery, pharmacy, and the food industry.**

As part of its component molding process for medical applications, our client encountered yellowing problems in a batch of material used on several pieces of equipment, a phenomenon that worsened during oven recoking. After initial internal investigations, FILAB was called in to understand the cause of the phenomenon.

## Summary

 01 Comparative studies: an essential methodology [](#cont-01) 02 Fourier transform infrared spectrometry [](#cont-02) 03 Why FILAB? [](#cont-03)   01
## Comparative studies: an essential methodology

When investigating failures, it is very helpful, where possible, to be able to compare the non-compliant sample with a compliant sample, i.e., one on which no degradation has been observed. This makes it possible to identify the source of a defect more quickly. In this case, our client was able to provide us with a sample from a compliant batch and then one from a non-compliant batch.

The first analytical hypothesis was that external contamination had impacted the formulation of the non-compliant batch. Here, we proposed to study organic contamination by GC-MS and inorganic contamination by ICP-AES.

The second hypothesis was to determine the thermal properties of the two materials to find out whether the non-compliant batch could have been affected by the process temperature. The data was obtained by thermogravimetric analysis (TGA).

These first two analytical approaches concluded that the yellowing was not caused by inorganic or organic contamination, nor by different behavior of the materials with respect to temperature. However, GC-MS revealed differences in formulation that had to be validated using additional analysis.

**A combination of several techniques is often necessary to understand a phenomenon**

![](https://filab.fr/wp-content/uploads/2022/09/spectres-atg.png)

ATG spectra of the different samples

   02
## Fourier transform infrared spectrometry

Fourier transform infrared spectroscopy (FTIR) is an analytical method commonly used to study polymers. It works by identifying the chemical bonds between the atoms that make up the polymer. It can also be used to detect abnormal degradation in a material by comparing degraded and new samples, or to characterize cross-linking mechanisms.

After studying the spectra, the FTIR analysis did not reveal any significant differences in composition.

![](https://filab.fr/wp-content/uploads/2022/09/spectres-irtf.png)

In addition to the results obtained previously, it was ultimately NMR spectroscopy, a technique that exploits the magnetic properties of certain atomic nuclei, that showed that the formulations of the two silicones were not equivalent. Here, NMR revealed, for example, that:

- The yellowing gum shows the presence of vinyl bonds, which are absent in the gum that remains white.
- The phenomenon of water absorption on the silica surface is also visible for the non-compliant sample, whereas it is not visible for the compliant silicone.
- The presence of higher quantities of carbon also probably contributes to the yellowing.
- Finally, silicon is more present in the non-compliant batch.

   03
## Why FILAB?

FILAB has extensive expertise and silicone characterization techniques tailored to a variety of needs, such as:

- Deformulation of unknown silicones
- Study of silicone thermal behavior using DSC or TGA
- Searching for impurities in silicone oils or fluids
- Expertise in silicone failures: odor, color, contamination, degradation issues, etc.

![](https://filab.fr/wp-content/uploads/2022/09/Meme-silicone-300x281.jpg)

  Need help? Contact our team [](#filab-contact-form)
## Other case studies you may be interested in

### Case study: goniometry and comparison of surface tensions

 One of our customers wanted to measure the contact angle and surface tension of their materials. [Learn more +](https://filab.fr/en/blog/2025/11/goniometry-and-comparison-of-surface-tensions.md)
### XPS coating

 Comparative study of multilayer coatings on zirconium tubes using XPS [Learn more +](https://filab.fr/en/blog/2025/12/study-of-the-purity-of-a-coating-layer-using-xps.md)
###

 [Learn more +](https://filab.fr/en/blog/2026/01/marking-problem-biopolymer-packaging.md) [View all our case studies](https://filab.fr/en/blog-filab.md)
## Services related to the case study

 [## Laboratory analysis of a joint](https://filab.fr/en/our-services/our-analysis-services/polymer-materials-analysis-laboratory/laboratory-analysis-of-joint.md) [## Deformulation of silicone in the laboratory](https://filab.fr/en/our-services/our-expertise-services/laboratory-deformulation-analysis-reverse-engineering/deformulation-silicone-laboratory.md) [## Deformulation of joint in the laboratory](https://filab.fr/en/our-services/our-expertise-services/laboratory-deformulation-analysis-reverse-engineering/deformulation-joint-laboratory.md) [## Laboratory of silicone testing and analysis](https://filab.fr/en/our-services/our-analysis-services/polymer-materials-analysis-laboratory/laboratory-analysis-silicone.md) [## Deformulation](https://filab.fr/en/our-services/our-expertise-services/laboratory-deformulation-analysis-reverse-engineering.md)   [![avis filab](https://filab.fr/wp-content/themes/astra-child/templates/assets/img/avis-verifies.svg) 5/5 ![note filab](https://filab.fr/wp-content/themes/astra-child/templates/assets/img/stars.svg)](https://www.avis-verifies.com/avis-clients/filab.fr)
## Laboratory specializing in analysis and expertise for industrial companies

 ![More than 140 people](https://filab.fr/wp-content/uploads/2024/10/collaborateurs-1.svg) More than 140 people at your service ![5200 m² laboratory](https://filab.fr/wp-content/uploads/2024/10/labo.svg) 5200 m² laboratory + 99% of services are provided in-house ![Accredited laboratory](https://filab.fr/wp-content/uploads/2024/10/ISO-17025-1.svg) Accredited laboratory COFRAC ISO 17025 ![+2200 clients](https://filab.fr/wp-content/uploads/2024/10/clients.svg) +2200 clients in France and abroad
### Contact us

 Our services are reserved for professionals.  [![phone](https://filab.fr/wp-content/themes/astra-child/templates/assets/img/form/phone.svg) Call
 us +33 (0)3 80 52 32 05](tel:+33380523205) [![location](https://filab.fr/wp-content/themes/astra-child/templates/assets/img/form/location.svg) Visit us 80 rue Jean-Louis Auguste Petitjean
 21850 - Saint Apollinaire - FRANCE](https://www.google.com/maps/place/Filab/@47.317329,5.076545,15z/data=!4m6!3m5!1s0x47f29e6ab37d6a1d:0xa2cc1016c4f74422!8m2!3d47.317793!4d5.0767354!16s%2Fg%2F1v3gr7f0?entry=ttu) [![mail](https://filab.fr/wp-content/themes/astra-child/templates/assets/img/form/envelope.svg) Contact
 us contact@filab.fr](mailto:contact@filab.fr?subject=%5BVotre%20demande%20:%20Understanding%20a%20marking%20problem%20on%20biopolymer%20packaging%20en%20%5D) For complaints: all complaints must be sent by mail to contact@filab.fr or by contacting the person who signed the report. The complaint handling procedure is available upon request. In the event of a complaint concerning the laboratory's activities, the customer may be notified of the complaint's handling.